Garment Processing Techniques for Fading Effects

Slide Note
Embed
Share

Learn about garment processing techniques such as PP Spray with Potassium Permanganate, P.P. Sponging, Tagging, and Destroy for creating unique fading effects on denim, twill, poplin, and corduroy garments. Follow safety precautions and specific procedures outlined for each technique.


Uploaded on Jul 18, 2024 | 0 Views


Download Presentation

Please find below an Image/Link to download the presentation.

The content on the website is provided AS IS for your information and personal use only. It may not be sold, licensed, or shared on other websites without obtaining consent from the author. Download presentation by click this link. If you encounter any issues during the download, it is possible that the publisher has removed the file from their server.

E N D

Presentation Transcript


  1. PP Spray (KMnO4: Potassium per Manganate Spray) 10 g KMnO4 in 1 litre 0r + Lubricant 1% and 5 g KMnO4 in 1 litre For pp spray, the garments are placed in a cabinet. Then KMnO4 solution is sprayed according to the requirement. After spraying the garments look grayish brown. Then it is neutralized with oxalic acid (COOH-COOH). Finally, faded (white) effect is produced. Cautions: -The worker must put on mask and hand gloves. -There must have back glass fountain system to avoid spreading of KMnO4 in air. -It is never done on grey garments. The garments must be desized before spraying.

  2. PP-Spray

  3. P.P SPONGING To import fading effect in specific areas (thigh, bum, knee) of garments as buyer recommended. P.P sponging is doing in Denim, Twill, Poplin, corduroy generally middle of wash i.e. after enzyme wash, stone enzyme wash. If need some area more white then we are doing P.P. sponging. Tools & Equipment: P.P. sponging operator must be used Hand gloves, Helmet, Mask, Ear plug &uniform for their safety.

  4. Process: We should take a rubber board on table. Place the rubbing board in side the leg panel. If need some particular area more white then we are doing P.P sponging. After P.P. sponging sodium metabisulphite is used to neutralize the garments. Standard stock solution for P.P. sponging is 0.4% i.e. 100 liter water 400 grams potassium permanganate. P.P sponging is done manually. By foam/ fabric pieces wet in p.p.stock solution and rubbing particular area of garments as result fading affects on garments. Application: The purpose of P.P sponging is also to create more fading affect on particular area of garments.

  5. Tagging

  6. Destroy Destroy is newly fashion on garments. Destroy is doing by manually. Different types of machine used for destroy the garments. When destroy is done one garment, it seems to be long time used effect. Grinding machine, emery cloth, hacksaw blade, knife etc. is used to destroy

  7. Procedure: We should take a pant on dummy. Direct apply knife/hacksaw blade, grinding machine. Needle is used when needed. As a result destroyed apparel will be produce. After this process wet process is needed. Application: This process is apply on normally bottom, pocket, opening in garments. Its produce fashionable garments.

Related